Cast Steel: The Iron-Carbon Equilibrium Diagram: Abstract
Cast Steel: The Iron-Carbon Equilibrium Diagram: Abstract
Diagram
Abstract:
A study of the constitution and structure of all steels and irons must first start
with the iron-carbon equilibrium diagram. Many of the basic features of this
system influence the behavior of even the most complex alloy steels.
For example, the phases found in the simple binary Fe-C system persist in
complex steels, but it is necessary to examine the effects alloying elements
have on the formation and properties of these phases. The iron-carbon
diagram provides a valuable foundation on which to build knowledge of both
plain carbon and alloy steels in their immense variety.
A study of the constitution and structure of all steels and irons must first start
with the iron-carbon equilibrium diagram. Many of the basic features of this
system (Fig. 1) influence the behavior of even the most complex alloy steels. For
example, the phases found in the simple binary Fe-C system persist in complex
steels, but it is necessary to examine the effects alloying elements have on the
formation and properties of these phases. The iron-carbon diagram provides a
valuable foundation on which to build knowledge of both plain carbon and alloy
steels in their immense variety.
It should first be pointed out that the normal equilibrium diagram really
represents the metastable equilibrium between iron and iron carbide (cementite).
Cementite is metastable, and the true equilibrium should be between iron and
graphite. Although graphite occurs extensively in cast irons (2-4 wt % C), it is
usually difficult to obtain this equilibrium phase in steels (0.03-1.5 wt %C).
Therefore, the metastable equilibrium between iron and iron carbide should be
considered, because it is relevant to the behavior of most steels in practice.
The much larger phase field of γ-iron (austenite) compared with that of α-iron
(ferrite) reflects the much greater solubility of carbon in γ-iron, with a maximum
value of just over 2 wt % at 1147°C (E, Fig.1). This high solubility of carbon in
γ-iron is of extreme importance in heat treatment, when solution treatment in the
γ-region followed by rapid quenching to room temperature allows a
supersaturated solid solution of carbon in iron to be formed.
The α-iron phase field is severely restricted, with a maximum carbon solubility
of 0.02 wt% at 723°C (P), so over the carbon range encountered in steels from
0.05 to 1.5 wt%, α-iron is normally associated with iron carbide in one form or
another. Similarly, the δ-phase field is very restricted between 1390 and 1534°C
and disappears completely when the carbon content reaches 0.5 wt% (B).
There are several temperatures or critical points in the diagram, which are
important, both from the basic and from the practical point of view.
• Firstly, there is the A1, temperature at which the eutectoid reaction occurs
(P-S-K), which is 723°C in the binary diagram.
• Secondly, there is the A3, temperature when α-iron transforms to γ-iron.
For pure iron this occurs at 910°C, but the transformation temperature is
progressively lowered along the line GS by the addition of carbon.
• The third point is A4 at which γ-iron transforms to δ-iron, 1390°C in pure
iron, hut this is raised as carbon is added. The A2, point is the Curie point
when iron changes from the ferro- to the paramagnetic condition. This
temperature is 769°C for pure iron, but no change in crystal structure is
involved. The A1, A3 and A4 points are easily detected by thermal
analysis or dilatometry during cooling or heating cycles, and some
hysteresis is observed. Consequently, three values for each point can be
obtained. Ac for heating, Ar for cooling and Ae (equilibrium}, but it
should be emphasized that the Ac and Ar values will be sensitive to the
rates of heating and cooling, as well as to the presence of alloying
elements.
The great difference in carbon solubility between γ- and α-iron leads normally to
the rejection of carbon as iron carbide at the boundaries of the γ phase field. The
transformation of γ to α - iron occurs via a eutectoid reaction, which plays a
dominant role in heat treatment.
Steels with less than about 0.8% carbon are thus hypo-eutectoid alloys with
ferrite and pearlite as the prime constituents, the relative volume fractions being
determined by the lever rule which states that as the carbon content is increased,
the volume percentage of pearlite increases, until it is 100% at the eutectoid
composition. Above 0.8% C, cementite becomes the hyper-eutectoid phase, and
a similar variation in volume fraction of cementite and pearlite occurs on this
side of the eutectoid composition.
The three phases, ferrite, cementite and pearlite are thus the principle
constituents of the infrastructure of plain carbon steels, provided they have been
subjected to relatively slow cooling rates to avoid the formation of metastable
phases.
Pearlite is probably the most familiar micro structural feature in the whole
science of metallography. It was discovered by Sorby over 100 years ago, who
correctly assumed it to be a lamellar mixture of iron and iron carbide.
These structures have much in common with the cellular precipitation reactions.
Both types of reaction occur by nucleation and growth, and are, therefore,
diffusion controlled. Pearlite nuclei occur on austenite grain boundaries, but it is
clear that they can also be associated with both pro-eutectoid ferrite and
cementite. In commercial steels, pearlite nodules can nucleate on inclusions.