Example 4
Example 4
VTT TECHNICAL RESEARCH Job Title ECSC Stainless Steel Valorisation Project
CENTRE OF FINLAND
VTT BUILDING AND TRANSPORT Subject Design Example 4 Fatigue strength of a welded
Kemistintie 3, Espoo hollow section joint
P.O.Box 1805, FIN02044 VTT, Finland
Telephone: + 358 9 4561
Client Made by AAT Date June 2002
Fax: + 358 9 456 7003
CALCULATION SHEET ECSC Checked by JEK Date June 2002
Revised by MEB Date April 2006
EN 1993-1-9:2005 is applicable to stainless steels for estimating the fatigue strength of Section 8
steel structures also. Therefore the section and clause references in this example are to EN
1993-1-9:2005.
The example shows the following design tasks for fatigue assessment:
- determination of the fatigue strength curve
- determination of secondary bending moments in the joint
- determination of the partial safety factor for fatigue strength and
- fatigue assessment for variable amplitude loading.
The chords of the joint are RHS 50x50x4 and braces RHS 30x30x2. The material is
grade 1.4301 stainless steel with 0,2% proof stress of 220 N/mm2.
11
30
x 30 x2
x2 2
x 30
30
50x50x4
Actions
Determined fatigue stress spectra for the chord during the required design life is:
Nominal stress range Number of cycles
131
Job No. R0SU00658 Sheet 2 of 3 Rev B
VTT TECHNICAL RESEARCH Job Title ECSC Stainless Steel Valorisation Project
CENTRE OF FINLAND
VTT BUILDING AND TRANSPORT Subject Design Example 4 Fatigue strength of a welded
Kemistintie 3, Espoo hollow section joint
P.O.Box 1805, FIN02044 VTT, Finland
Telephone: + 358 9 4561
Client Made by AAT Date June 2002
Fax: + 358 9 456 7003
CALCULATION SHEET ECSC Checked by JEK Date June 2002
Revised by MEB Date April 2006
Fatigue assessment
Reference stress range corresponding 2 106 stress fluctuations for detail category 71 is:
c = 71 N/mm2
The fatigue strength curve for lattice girders has a constant slope m = 5 Figure 7.1
The number of stress fluctuations corresponding nominal stress range i is
m
6 c
Ni = 2 10 and
Mf Ff (k1,0 i )
1 = 100 N/mm 2 N1 = 47,5 103
2 = 70 N/mm2 N 2 = 283 103
3 = 40 N/mm2 N 3 = 4640 103
132
Job No. R0SU00658 Sheet 3 of 3 Rev B
VTT TECHNICAL RESEARCH Job Title ECSC Stainless Steel Valorisation Project
CENTRE OF FINLAND
VTT BUILDING AND TRANSPORT Subject Design Example 4 Fatigue strength of a welded
Kemistintie 3, Espoo hollow section joint
P.O.Box 1805, FIN02044 VTT, Finland
Telephone: + 358 9 4561
Client Made by AAT Date June 2002
Fax: + 358 9 456 7003
CALCULATION SHEET ECSC Checked by JEK Date June 2002
Revised by MEB Date April 2006
n A.5 (1)
n Ei
The cumulative damage during the design life Dd = N Ri
= Dd,i = 0,78
i
Because the cumulative damage is less than unity, the calculated design life of the chord is Clause 8(4)
more than the required design life.
The procedure described above shall also be repeated for the brace.
133
BLANK PAGE
134