0% found this document useful (0 votes)
74 views

Politeknik Negeri Pontianak: Laboratorium Teknik Sipil

The document appears to be a laboratory report from the Civil Engineering Laboratory at the Pontianak State Polytechnic detailing the results of a concrete compression test. It includes information on the project, materials used, test date, specimen measurements and weights, applied loads, and compressive strength test results. The concrete achieved an average compressive strength of 81.4 kg/cm2.

Uploaded by

Muhammad Andre
Copyright
© © All Rights Reserved
We take content rights seriously. If you suspect this is your content, claim it here.
Available Formats
Download as XLS, PDF, TXT or read online on Scribd
0% found this document useful (0 votes)
74 views

Politeknik Negeri Pontianak: Laboratorium Teknik Sipil

The document appears to be a laboratory report from the Civil Engineering Laboratory at the Pontianak State Polytechnic detailing the results of a concrete compression test. It includes information on the project, materials used, test date, specimen measurements and weights, applied loads, and compressive strength test results. The concrete achieved an average compressive strength of 81.4 kg/cm2.

Uploaded by

Muhammad Andre
Copyright
© © All Rights Reserved
We take content rights seriously. If you suspect this is your content, claim it here.
Available Formats
Download as XLS, PDF, TXT or read online on Scribd
You are on page 1/ 20

KEMENTERIAN PENDIDIKAN NASIONAL

POLITEKNIK NEGERI PONTIANAK


LABORATORIUM TEKNIK SIPIL

ANALISA AYAK / SIEVE ANALYSIS


PB - 0201 - 76

Jenis Material : Sumber :


Pekerjaan :
Berat Contoh : gr

DIAMETER Berat Masing2 Berat Tertahan Persen


% KUMULATIF
AYAKAN Tertahan Kumulatif Tertahan Spesifikasi
Inch mm (gram) (gram) (%) Tertahan Lolos
3 76.20 0.00 0.00 #DIV/0! #DIV/0! #DIV/0!
2 50.80 0.00 0.00 #DIV/0! #DIV/0! #DIV/0!
1 1/2 38.00 0.00 0.00 #DIV/0! #DIV/0! #DIV/0!
1 1/4 31.50 0.00 0.00 #DIV/0! #DIV/0! #DIV/0!
1 25.40 0.00 0.00 #DIV/0! #DIV/0! #DIV/0!
3/4 19.10 0.00 0.00 #DIV/0! #DIV/0! #DIV/0!
5/8 16.00 0.00 0.00 #DIV/0! #DIV/0! #DIV/0!
1/2 12.70 0.00 0.00 #DIV/0! #DIV/0! #DIV/0!
3/8 9.50 0.00 0.00 #DIV/0! #DIV/0! #DIV/0!
No. 4 4.750
No. 8 2.360
No. 16 1.180
No. 30 0.600
No. 50 0.300
No. 100 0.150
No. 200 0.075
Pan 0
Jumlah

100
Persen Lolos (%)

80

60

40

20

0
0.010 0.100 1.000 10.000 100.000
Diameter Ayak (mm)
4.750
2.360
1.180
0.600
0.300
0.150
0.075
99.740
100.00
KEMENTERIAN PENDIDIKAN NASIONAL
POLITEKNIK NEGERI PONTIANAK
LABORATORIUM TEKNIK SIPIL

Laporan Hasil Pengujian Beton


Uji Kuat Tekan Kubus / Silinder

Proyek : Tugas Akhir Semen Portland : 5,975 kg Type :


Air : 3,7085 l dari : Lab. Teknik Sipil
Pekerjaan : Pengujian Beton Pasir Halus : 12,600 kg dari : Lab. Teknik Sipil
Pelaksana : Fikriandry dan Ryanda Kerang Ale-Ale : 298,75 g dari : Kab. Ketapang
Lokasi : Lab. Teknik Sipil Polnep Kerikil (Batu Pecah) : 19,300 kg dari : Lab. Teknik Sipil

Tanggal Pengujian : 21-Jul-17


Angka Kalibrasi Alat :
Angka Korelasi Bentuk : 0.83
Penggunaan Additif : Tidak

n ti n ti n ti umur angka
3 2.940 10 1.833 17 1.746 (hari) korelasi
4 2.353 11 1.812 18 1.740 3 0.40
5 2.132 12 1.796 19 1.734 7 0.65
6 2.015 13 1.782 20 1.729 14 0.88
7 1.943 14 1.771 21 0.95
8 1.895 15 1.761 28 1.00
9 1.860 16 1.753
ti = faktor koreksi terhadap jumlah benda uji

Tanggal Umur Ukuran Berat Beban P Beban Kuat Tekan Angka Kuat Tekan (sb' - sbm') (sb' - sbm')2
No Kode Pembuatan/ (15x15) x Kalibrasi sb' Korelasi 28 hari
Pengecoran ( hari ) (cm2) ( kg ) ( KN ) ( kg ) ( kg/cm2 ) ( kg/cm2 ) ( kg/cm2 ) ( kg/cm2 )

1 1-5-175 17/2/2011 3 176.71 12.90 100 8461.0 47.88 0.40 119.70 38.30 1467.25
2 2-5-175 17/2/2011 3 176.71 12.70 100 8461.0 47.88 0.40 119.70 38.30 1467.25
3 3-5-175 17/2/2011 3 176.71 12.40 140 11845.4 67.03 0.40 167.58 86.19 7427.94

406.99 10362.43

n
b '
bm ' = = 81.4 kg/cm2

1 n

( b' bm ' )2
n
SD = n1
= 72.0 kg/cm2

ti x SD
bk ' = bm ' = -2.3 kg/cm2
n
KEMENTERIAN PENDIDIKAN NASIONAL
POLITEKNIK NEGERI PONTIANAK
LABORATORIUM TEKNIK SIPIL

Laporan Hasil Pengujian Beton


Uji Kuat Tekan Kubus / Silinder

Proyek : Tugas Akhir Semen Portland : 5,975 kg Type :


Air : 3,7085 l dari : Lab. Teknik Sipil
Pekerjaan : Pengujian Beton Pasir Halus : 12,600 kg dari : Lab. Teknik Sipil
Pelaksana : Fikriandry dan Ryanda Kerang Ale-Ale : 896,25 g dari : Kab. Ketapang
Lokasi : Lab. Teknik Sipil Polnep Kerikil (Batu Pecah) : 19,300 kg dari : Lab. Teknik Sipil

Tanggal Pengujian : 21-Jul-17


Angka Kalibrasi Alat :
Angka Korelasi Bentuk : 0.83
Penggunaan Additif : Tidak

n ti n ti n ti umur angka
3 2.940 10 1.833 17 1.746 (hari) korelasi
4 2.353 11 1.812 18 1.740 3 0.40
5 2.132 12 1.796 19 1.734 7 0.65
6 2.015 13 1.782 20 1.729 14 0.88
7 1.943 14 1.771 21 0.95
8 1.895 15 1.761 28 1.00
9 1.860 16 1.753
ti = faktor koreksi terhadap jumlah benda uji

Tanggal Umur Ukuran Berat Beban P Beban Kuat Tekan Angka Kuat Tekan (sb' - sbm') (sb' - sbm')2
No Kode Pembuatan/ (15x15) x Kalibrasi sb' Korelasi 28 hari
Pengecoran ( hari ) (cm2) ( kg ) ( KN ) ( kg ) ( kg/cm2 ) ( kg/cm2 ) ( kg/cm2 ) ( kg/cm2 )

1 1-5-175 17/2/2011 3 176.71 12.50 105 8884.1 50.27 0.40 125.69 38.30 1467.25
2 2-5-175 17/2/2011 3 176.71 12.60 120 10153.2 57.46 0.40 143.64 56.26 3165.18
3 3-5-175 17/2/2011 3 176.71 12.90 140 11845.4 67.03 0.40 167.58 80.20 6432.10

436.91 11064.53

n
b '
bm ' = = 87.4 kg/cm2

1 n

( b' bm ' )2
n
SD = n1
= 74.4 kg/cm2

ti x SD
bk ' = bm ' = 0.9 kg/cm2
n
KEMENTERIAN PENDIDIKAN NASIONAL
POLITEKNIK NEGERI PONTIANAK
LABORATORIUM TEKNIK SIPIL

Laporan Hasil Pengujian Beton


Uji Kuat Tekan Kubus / Silinder

Proyek : Tugas Akhir Semen Portland : 5,975 kg Type :


Air : 3,7085 l dari : Lab. Teknik Sipil
Pekerjaan : Pengujian Beton Pasir Halus : 12,600 kg dari : Lab. Teknik Sipil
Pelaksana : Fikriandry dan Ryanda Kerang Ale-Ale : 597,5 g dari : Kab. Ketapang
Lokasi : Lab. Teknik Sipil Polnep Kerikil (Batu Pecah) : 19,300 kg dari : Lab. Teknik Sipil

Tanggal Pengujian : 24-Jul-17


Angka Kalibrasi Alat :
Angka Korelasi Bentuk : 0.83
Penggunaan Additif : Tidak

n ti n ti n ti umur angka
3 2.940 10 1.833 17 1.746 (hari) korelasi
4 2.353 11 1.812 18 1.740 3 0.40
5 2.132 12 1.796 19 1.734 7 0.65
6 2.015 13 1.782 20 1.729 14 0.88
7 1.943 14 1.771 21 0.95
8 1.895 15 1.761 28 1.00
9 1.860 16 1.753
ti = faktor koreksi terhadap jumlah benda uji

Tanggal Umur Ukuran Berat Beban P Beban Kuat Tekan Angka Kuat Tekan (sb' - sbm') (sb' - sbm')2
No Kode Pembuatan/ (15x15) x Kalibrasi sb' Korelasi 28 hari
Pengecoran ( hari ) (cm2) ( kg ) ( KN ) ( kg ) ( kg/cm2 ) ( kg/cm2 ) ( kg/cm2 ) ( kg/cm2 )

1 1-5-175 17/2/2011 5 176.71 12.00 80 6768.8 38.30 0.53 72.27 10.84 117.53
2 2-5-175 17/2/2011 5 176.71 12.10 160 13537.6 76.61 0.53 144.55 83.11 6907.92
3 3-5-175 17/2/2011 5 176.71 11.90 100 8461.0 47.88 0.53 90.34 28.91 835.74

307.16 7861.18

n
b '
bm ' = = 61.4 kg/cm2

1 n

( b' bm ' )2
n
SD = n1
= 62.7 kg/cm2

ti x SD
bk ' = bm ' = -11.5 kg/cm2
n
Job Mix Formula Beton K-225

KEMENTERIAN PENDIDIKAN NASIONAL


POLITEKNIK NEGERI PONTIANAK
LABORATORIUM TEKNIK SIPIL

HASIL UJI SLUMP

Proyek :

Lokasi :

Pekerjaan :
Material
Semen :
Pasir :
Kerikil :
Air : PDAM

Pemeriksaan Slump (mm)


1 135.0
2 140.0
3 160.0
Rata-rata 145.0
Job Mix Formula Beton K-225

KEMENTERIAN PENDIDIKAN NASIONAL


POLITEKNIK NEGERI PONTIANAK
LABORATORIUM TEKNIK SIPIL

HASIL UJI SLUMP

Proyek :

Lokasi :

Pekerjaan :
Material
Semen :
Pasir :
Kerikil :
Air : PDAM

Pemeriksaan Slump (mm)


1 130.0
2 190.0
3 210.0
Rata-rata 176.7
Job Mix Formula Beton K-225

KEMENTERIAN PENDIDIKAN NASIONAL


POLITEKNIK NEGERI PONTIANAK
LABORATORIUM TEKNIK SIPIL

HASIL UJI SLUMP

Proyek :

Lokasi :

Pekerjaan :
Material
Semen :
Pasir :
Kerikil :
Air : PDAM

Pemeriksaan Slump (mm)


1 130.0
2 200.0
3 200.0
Rata-rata 176.7
Job Mix Formula Beton K-225

KEMENTERIAN PENDIDIKAN NASIONAL


POLITEKNIK NEGERI PONTIANAK
LABORATORIUM TEKNIK SIPIL

HASIL UJI SLUMP

Proyek :

Lokasi :

Pekerjaan :
Material
Semen :
Pasir :
Kerikil :
Air : PDAM

Pemeriksaan Slump (mm)


1 100.0
2 200.0
3 250.0
Rata-rata 183.3
Job Mix Formula Beton K-225

KEMENTERIAN PENDIDIKAN NASIONAL


POLITEKNIK NEGERI PONTIANAK
LABORATORIUM TEKNIK SIPIL

Proyek :

Lokasi :

Pekerjaan :

REKAPITULASI HASIL PENGUJIAN LABORATORIUM

Jenis Bahan
No. Jenis Pengujian Satuan
Agregat Halus Agregat Kasar

1 Analisa Saringan
2 Besar Butir Maksimum mm
3 Berat Jenis SSD
4 Penyerapan Air %
5 Berat Isi Effektif gr/cm3
KEMENTERIAN PENDIDIKAN NASIONAL
POLITEKNIK NEGERI PONTIANAK
LABORATORIUM TEKNIK SIPIL

HASIL UJI KADAR AIR AGREGAT KASAR

Jenis Material : Batu Sumber : Lab.Teknik Sipil Polnep

PEMERIKSAAN I II
No. cawan 1 2
Berat cawan ( W1 ) 544.00 543.00
Berat cawan + benda uji ( W2 ) 6619.00 6359.00
Berat benda uji ( W3 = W2 - W1 ) 6077.00 5816.00
Berat cawan + benda uji kering oven ( W4 ) 6019.00 6347.00
Berat benda uji kering oven ( W5 = W4 - W1 ) 6075.00 5804.00

PEMERIKSAAN I II Rata-rata

Kadar air agregat ( W3 W5 ) 0.03 0.21 0.12


= 100
W5

HASIL UJI KADAR AIR AGREGAT HALUS

Jenis Material : Pasir Sumber : Lab.Teknik Sipil Polnep


PEMERIKSAAN I II
No. cawan 1 2
Berat cawan ( W1 ) 717.00 552.00
Berat cawan + benda uji ( W2 ) 6615.00 6956.00
Berat benda uji ( W3 = W2 - W1 ) 5898.00 6404.00
Berat cawan + benda uji kering oven ( W4 ) 6580.00 6947.00
Berat benda uji kering oven ( W5 = W4 - W1 ) 5863.00 6395.00

PEMERIKSAAN I II Rata-rata

Kadar air agregat ( W3 W5 ) 0.597 0.141 0.369


= 100
W5
KEMENTERIAN PENDIDIKAN NASIONAL
POLITEKNIK NEGERI PONTIANAK
LABORATORIUM TEKNIK SIPIL

BERAT JENIS DAN PENYERAPAN AGREGAT KASAR

Jenis Material : Batu Sumber : Lab.Teknik Sipil Polnep

PEMERIKSAAN I II
Berat benda uji jenuh permukaan kering ( Bj ) (gram) 502 502
Berat benda uji kering oven ( B2 ) (gram) 500 500
Berat bejana berisi air ( B3 ) (gram) 1313 1313
Berat bejana + benda uji + air ( B1 ) (gram) 1623 1628

PEMERIKSAAN I II Rata-rata

Berat jenis bulk/ov. B2 2.61 2.67 2.64


=
B3 + Bj B1

Berat jenis SSD


Bj
= 2.62 2.68 2.65
B3 + Bj B1

Berat jenis app. B2 2.63 2.70 2.67


=
B3 + B2 B1

Penyerapan Bj B2 0.37 0.36 0.37


= 100
B2
KEMENTERIAN PENDIDIKAN NASIONAL
POLITEKNIK NEGERI PONTIANAK
LABORATORIUM TEKNIK SIPIL

HASIL UJI BERAT ISI AGREGAT

Jenis Material: Batu Sumber : Lab.Teknik Sipil Polnep

Padat Lepas
PEMERIKSAAN
I II I II
Berat Mould ( W1 ) 2156.00 2156.00 2156.00 2156.00
Berat Mould + benda uji ( W2 ) 7530.00 7533.00 7187.00 7259.00
Berat benda uji ( W3 = W2 - W1 ) 5374.00 5377.00 5031.00 5103.00
Berat Mould + air ( W4 ) 5262.00 5262.00 5262.00 5262.00
Berat air / Isi Mould ( V = W4 - W1 ) 3106.00 3106.00 3106.00 3106.00

PEMERIKSAAN

Berat Isi W3
= ( kg/dm3 ) 1.730 1.731 1.620 1.643
V
Rata-rata 1.731 1.631
Rata-rata 1.681

Jenis Material: Pasir Sumber : Lab.Teknik Sipil Polnep

Padat Lepas
PEMERIKSAAN
I II I II
Berat Mould ( W1 ) 2156.00 2156.00 2156.00 2156.00
Berat Mould + benda uji ( W2 ) 6890.00 6780.00 6410.00 6705.00
Berat benda uji ( W3 = W2 - W1 ) 4734.00 4624.00 4254.00 4247.00
Berat Mould + air ( W4 ) 5262.00 5262.00 5262.00 5262.00
Berat air / Isi Mould ( V = W4 - W1 ) 3106.00 3106.00 3106.00 3106.00

PEMERIKSAAN

Berat Isi W3
= ( kg/dm3 ) 1.524 1.489 1.370 1.367
V
Rata-rata 1.506 1.368
Rata-rata 1.437
KEMENTERIAN PENDIDIKAN NASIONAL
POLITEKNIK NEGERI PONTIANAK
LABORATORIUM TEKNIK SIPIL

BERAT JENIS DAN PENYERAPAN AGREGAT HALUS

Jenis Material : Pasir Sumber : Lab.Teknik Sipil Polnep

PEMERIKSAAN I II
Berat benda uji jenuh permukaan kering ( SSD ) (gram) 500 500
Berat benda uji kering oven ( B2 ) (gram) 496 496
Berat bejana berisi air ( B3 ) (gram) 858 858
Berat bejana + benda uji + air ( B1 ) (gram) 1166 1164

PEMERIKSAAN I II Rata-rata

B2
Berat jenis bulk/ov. = 2.58 2.56 2.57
B3 + SSD B1

Berat jenis SSD SSD 2.60 2.58 2.59


=
B3 + SSD B1

Berat jenis app.


B2 2.64 2.61 2.63
=
B3 + B2 B1

Penyerapan
SSD - B2
= x 100 % 0.93 0.82 0.88
B2
KEMENTERIAN PENDIDIKAN NASIONAL
POLITEKNIK NEGERI PONTIANAK
LABORATORIUM TEKNIK SIPIL

ANALISA AYAK / SIEVE ANALYSIS


PB - 0201 - 76

Jenis Material : Agg. Kasar Sumber : Lab.Teknik Sipil Polnep


Pekerjaan :
Berat Contoh : gr

DIAMETER Berat Masing2 Berat Tertahan Persen


% KUMULATIF
AYAKAN Tertahan Kumulatif Tertahan Spesifikasi
Inch mm (gram) (gram) (%) Tertahan Lolos
3 76.20 0.00 0.00 0.00 0.00 100.00
2 50.80 0.00 0.00 0.00 0.00 100.00
1 1/2 38.00
1 1/4 31.50
1 25.40 0.00 0.00 0.00 0.00 100.00
3/4 19.10 2364.50 2364.50 29.29 29.29 70.71
5/8 16.00 3011.00 5375.50 37.30 66.59 33.41
1/2 12.70 839.50 6215.00 10.40 76.99 23.01
3/8 9.50 1291.00 7506.00 15.99 92.98 7.02
No. 4 4.750 566.50 8072.50 7.02 100.00 0.00
No. 8 2.360 0.00 0.00 100.00 0.00
No. 16 1.180 0.00 0.00 100.00 0.00
No. 30 0.600 0.00 0.00 100.00 0.00
No. 50 0.300 0.00 0.00 100.00 0.00
No. 100 0.150 0.00 0.00 100.00 0.00
No. 200 0.075 0.00 0.00 100.00 0.00
Pan 0 0.60 8073.10 0.01 100.00 0.00
Jumlah 8073.10

100.00
Persen Lolos (%)

80.00

60.00

40.00

20.00

0.00
1.00 10.00 100.00
Diameter Ayak (mm)
31.50 94.31
25.40 57.86
19.10 5.83
16.00 1.39
12.70 0.03
9.50 0.03
4.750 0.01
KEMENTERIAN PENDIDIKAN NASIONAL
POLITEKNIK NEGERI PONTIANAK
LABORATORIUM TEKNIK SIPIL

ANALISA AYAK / SIEVE ANALYSIS


PB - 0201 - 76

Jenis Material : Agg. Halus Sumber : Lab.Teknik Sipil Polnep


Pekerjaan :
Berat Contoh : gr

DIAMETER Berat Masing2 Berat Tertahan Persen


% KUMULATIF
AYAKAN Tertahan Kumulatif Tertahan Spesifikasi
Inch mm (gram) (gram) (%) Tertahan Lolos
3 76.20 0.00 0.00 0.00 0.00 100.00
2 50.80 0.00 0.00 0.00 0.00 100.00
1 1/2 38.00 0.00 0.00 0.00 0.00 100.00
1 1/4 31.50 0.00 0.00 0.00 0.00 100.00
1 25.40 0.00 0.00 0.00 0.00 100.00
3/4 19.10 0.00 0.00 0.00 0.00 100.00
5/8 16.00 0.00 0.00 0.00 0.00 100.00
1/2 12.70 0.00 0.00 0.00 0.00 100.00
3/8 9.50 0.00 0.00 0.00 0.00 100.00
No. 4 4.750 5.66 5.66 1.13 1.13 98.87
No. 8 2.360 16.00 21.65 3.21 4.34 95.66
No. 16 1.180 94.49 116.14 18.96 23.30 76.70
No. 30 0.600 194.52 310.66 39.04 62.34 37.66
No. 50 0.300 97.42 408.07 19.55 81.89 18.11
No. 100 0.150 69.27 477.34 13.90 95.79 4.21
No. 200 0.075 16.54 493.87 3.32 99.11 0.89
Pan 0 4.31 498.18 0.86 99.98 0.02
Jumlah 498.18 99.98

100.00
Persen Lolos (%)

80.00

60.00

40.00

20.00

0.00
0.010 0.100 1.000 10.000 100.000
Diameter Ayak (mm)
4.750 99.86
2.360 99.22
1.180 94.88
0.600 31.18
0.300 3.42
0.150 0.96
0.075 0.26
99.740
100.00 0.00
KEMENTERIAN PENDIDIKAN NASIONAL
POLITEKNIK NEGERI PONTIANAK
LABORATORIUM TEKNIK SIPIL

Laporan Hasil Pengujian Beton


Alat Uji Hammer Test

Lokasi : Tanggal :
Jenis Struktur : Diuji Oleh :
kondisi :

No.Titik Rebound Value Impact Angle Standard Value Ccef. Of Concrete Age
Raverage R
Sampel 1 2 3 () (R0) (n)
52 48 48
Kolom 38 54 48 46.22 0 0 46.22 0.8
38 40 50

30 28 30
Lantai 26 25 26 28 -90 +4 32 0.8
28 28 31

60 57 50
Tangga 54 56 52 53 +45 -2,7 #VALUE! 0.63
54 54 40

44 42 36
Balok 46 39 37 40.89 0 0 40.89 0.63
40 40 44
Comp.Strength (F)
(kg/cm2)

333.51

185.60

#VALUE!

218.96