BASF Injection Molding Defects PDF
BASF Injection Molding Defects PDF
in styrene copolymers
and their prevention
4 I. Injection molding faults
1. Streaks
1.1 Moisture streaks/splay marks
1.2 Burning streaks/silver streaks
1.3 Dark streaks due to indrawn air
1.3 Color streaks
8 2. Peeling/delamination
3. Weld lines
10 4. Air entrapments/bubble formation
12 5. Sink marks
6. Voids
14 7. Glossy spots or differences in gloss/mat spots
16 8. Microcracks, crazing, stress whitening
18 9. Diesel effect
20 10. Demolding problems
22 11. Push marks (tiger stripes/tiger lines)
24 12. Record effect
26 13. Short shot
28 14. Flash formation
30 15. Jetting
32 16. Cold slug
34 17. Warpage
3
I. Injection molding faults
1. Streaks
1.1 Moisture streaks/splay marks
Appearance Cause Correction
Usually oblong, silvery surface Moisture content too high; water vapor is produced dur- 1. Use material adequately predried to a residual mois-
streaks which are open in the ing melting and this results in the surface of the molding ture content of < 0.1 %.
shape of a U counter to the being torn open.
direction of flow. The material 2. Increase back pressure.
pumped out of the cylinder is
foamed and shows blisters on
the surface.
Silvery or dark surface streaks 1. Damage to the plastic melt due to excessively high 1. Reduction of the injection speed.
and in exceptional cases black temperatures or overlong residence times resulting
discolorations. from gaseous decomposition products.
2. High shear heating due to small gate cross sections or 2. Avoidance of undersized gates and sharp changes in
by sharp changes of direction in the mold. direction (shear intensive areas) in the mold.
3. Check the controller of the hot runner system and the
barrel heater.
4. Reduction of melt temperature, screw speed (rpm),
residence time (if necessary use a smaller plasticizing
unit) and back pressure.
4
1.1 Moisture streaks 1.2 Burning streaks
Sprue
Streaks ranging in color from 1. Processing using a screw which is too deeply flighted 1. Raise temperature in feed section so that melting is
dark to black in the feed section (air intake). earlier; use more suitable screw.
2. Dead spots in the plasticising unit or hot runner 2. Check plasticizing unit and hot runners for zones of
system. impeded flow and if necessary correct them.
3. Defective nonreturn valve. 3. Replace defective nonreturn valve.
4. Screw decompression is too great or too fast. 4. Shorten the path for screw decompression or
decompress at a reduced rate.
Color differences 1. Inhomogeneous distribution of colorant; accumulations 1. Use of suitable colorants and batches; ensure good
of colorant; unsuitable color batch; alignment / homogenization and dispersion; avoid thermal over-
orientation of the usually inorganic pigments by flow loading.
processes; thermal pigment damage.
2. Dead spots in the plasticising unit or hot runner system. 2. Avoid dead spots in the plasticising unit and in the
hot runner system.
3. Contamination 3. Make sure a good cleaning of the plasticising unit.
The cause for the formation of streaks can be deter- Melt temperature
mined in many cases only after costly investigations, Injection speed
especially as the appearance of burning and moisture Residence time in the cylinder
streaks is similar. Extensive knowledge of the plastic, Back pressure
the mold design and the processing are indispensable
Moisture content of granules
for overcoming the problem. Before launching expen-
sive and time-consuming investigations the following Mold venting
points should be checked in the sequence given and Cleaning of the plasticising unit
if necessary optimized: Screw recovery speed
6
1.3 Dark streaks 1.4 Color streaks
Fig. 1.3.1: Dark streaks caused by deposits of thermally damaged material Fig. 1.4.2: Color streaks due to deposits of material due to dead spots in a
from the hot runner hot runner system
Fig. 1.4.1: Color streaks (inhomogeneous distribution of colorant) Fig. 1.4.3: Color streaks in transmitted light; magnification 7:1
7
2. Peeling/Delamination
Appearance Cause Correction
Detached, slate-like surface 1. High shear stresses result in the formation of layers; 1. Increase the melt temperature and reduce the injection
layers, e.g. due to cross cutting; even in compatible multiphase systems. speed.
usually not easy to identify
since the surface is flawless; a
2. Contamination with an incompatible thermoplastic or 2. Avoid contamination due to extraneous material or due
skin can often be pulled off
master batch. to an unsuitable master batch (specifically the carrier).
when the surface is scratched
with a blade. The molded part
exhibits bubbling after warm
storage.
3. Weld line
Appearance Cause Correction
Notches, hairlines Appear in multiphase systems such as ABS or ASA. Flow As far as possible, position weld lines where they have no
fronts having an already cooled peripheral layer visual or mechanical impact (flow promoters, flow
encounter one another and no longer allow fusion without inhibitors); check mold engineering: if necessary enlarge
marks. sprue channel, gate and machine nozzle; avoidance of
aprupt changes in wall thickness and nonuniform mold
filling; provide effective mold venting.
Change in apparent color; espe- Decorative effect pigments and, e. g., glass fibers tend to
cially when inorganic decorative straighten up in the region of the weld line (adversely Processing: Optimization of melt temperature, mold sur-
effect pigments are used the affecting appearance and usually mechanical properties face temperature and injection speed; new color formula-
weld line appears as a dark line; also). tion (organic or inorganic pigments, higher pigmentation).
conspicuous in dark, brilliant or
transparent moldings having
smooth surfaces polished to a Use lower viscosity material.
high gloss.
8
2. Peeling/Delamination 3. Weld line
Position 1
1.5 mm
Position 2
Fig. 3.3: Weld line (metallic effect Fig. 3.4: Color marking in the
coloring) weld line; vertical illumination,
dark field, magnification 52:1
Fig. 2.4: Position 2
9
4. Air entrapments/bubble formation
The air entrapped during injec- 1. During mold filling air is entrapped on account of an 1. As far as necessary optimize the geometry of the
tion of the melt is visible as a inopportune shape of the molding and if occluded in molding with the aid of a mold flow calculation.
cavity (air bubble) in the molded the peripheral region close to the surface this can give
part. Air entrapments should rise to bubbles.
not be confused with voids. 2. Check design and condition of mold vents.
10
4. Air entrapments (bubble formation)
(front elevation and section)
Air bubble
Depressions on the surface of Sink marks are always produced in regions of accumula- Avoid large differences in wall thickness and accumula-
the molded part. tion of material when the contraction in volume arising tions of material (e.g. by means of rib structures having
during the cooling phase cannot be adequately compen- large radii, fixing domes, etc.); a rib thickness of 0.5 - 0.7
sated for by the holding pressure. times the basic wall thickness is advantageous.
Optimize melt and mold temperature; set the holding
pressure, holding pressure time and melt cushion to ade-
quate dimensions (increase values).
As far as possible gate at the greatest wall thickness;
design the sprue and gate cross sections in keeping with
the material and molded part.
Cool thick-walled parts in cold water (freezing of the
peripheral layer) in order to shorten the setting time.
6. Voids
Appearance Cause Correction
Usually not discernible from the As for Item 5. Avoid large differences in wall thickness and accumula-
outside except in the case of tions of material (e.g. by means of rib structures having
Exception: When the outer skin is thick enough to absorb large radii, fixing domes, etc.).
transparent materials. the shrinkage stresses.
Parts, usually thick-walled, Pay heed to correct temperature control; set the holding
The melt in the interior is pulled towards the outside pressure, holding pressure time and melt cushion to
which have been cut open (molding surface) so that vacuum cavities are produced
reveal cavities. adequate dimensions.
in the region which is still plastic.
As far as possible gate in the thickwalled area; design
This occurs only when the molding has cooled for long the sprue and gate cross sections in keeping with the
enough. material and molded part.
12
5. Sink marks 6. Voids
(front elevation and section)
Melt accumulation
13
7. Glossy spots or differences in gloss/mat spots
Appearance Cause Correction
Injected parts generally having 1. As a result of design related material accumulations, 1. Avoid material accumulations and aprupt changes in
a gloss which is too low or too such as aprupt changes in wall thickness, ribs and wall thickness; gate the part in the thickwalled area.
high. fixing bosses sink marks are produced which give
rise to glossy spots in textured surfaces.
Nonuniform apparent gloss or
color at certain areas. 2. Mat spots often arise on glossy parts having complex 2. Optimize the part and mold filling, e.g. injection
geometry (aprupt changes in wall thickness, ribs, profile (multistage injection). Polish the finished part.
openings) when at the same time the mold filling
process is unsatisfactory.
3. On weld lines due e.g. to alignments and changed 3. As far as possible position weld lines where they are not
flow conditions. visible (flow promoters, flow inhibitors); mold flow
studies also provide guidance.
4. Sprue and gate cross sections are too small. 4. Have adequately sized sprue and gate cross sections.
5. Mold wall temperature, melt temperature and injection 5. Optimize the processing temperature. Check the mold
speed are not favorable. cooling and coolant flow.
6. Holding pressure and holding pressure time are too low. 6. Adjust holding pressure and holding pressure time.
14
7. Glossy spots or differences in gloss/mat spots Fig. 7.2: High Fig. 7.4: Poor
(Automobile mirror mounting) reproduction reproduction
accuracy accuracy
(mat); scan- (glossy); scan-
ning electron ning electron
micrograph, micrograph,
Fig. 7.1: magnification magnification
Differences in 50:1 50:1
gloss on account
of good (mat) or Fig. 7.3: High Fig. 7.5: Poor
poor (glossy) mold reproduction reproduction
reproduction accuracy accuracy
mat glossy
(mat); scan- (glossy); scan-
ning electron ning electron
micrograph, micrograph,
magnification magnification
200:1 200:1
15
8. Microcracks, crazing and stress whitening
Appearance Cause Correction
Milky to whitish cloudiness Due to exceeding the maximum permissible yield point as
(incident light is scattered dif- a result of the following for example.
fusely).
1. Action of external force, arising for example from 1. Reduce the force acting on the molding from the outside
forcible demolding of undercuts. or employ thermoplastics having lower susceptibility to
stress whitening e.g. Luran S (ASA) optimize the molddesign.
3. Internal stresses in the part due to inappropriate 3. Increase mold surface and melt temperatures, reduce
processing conditions. holding pressure and setting times and adjust injection
speed; aim for low-stress processing in line with the
requirements of the material; do not demold under
residual pressure; select the ejector mechanisms and
demolding drafts in such a way that troublefree demold-
ing without relatively great force is ensured; alteration of
sprue and gate conditions; modification of part design.
4. Use of mold release sprays which may, for example, 4. Employ suitable demolding aids.
cause stress cracking.
16
8. Microcracks, crazing and stress whitening
a)
b)
Fig. 8.2:
a) Ballpoint pen with stress whitening in the thread region
(undercut) made from pure polybutadiene ABS
b) The same ballpoint pen without stress whitening made from Luran S (ASA)
a b
Fig. 8.1: Microcracks produced by overloading and deforming under residual Fig. 8.3: Terluran (967 K) Luran S (ASA)
pressure
17
9. Diesel effect
Appearance Cause Correction
Scorching or black colorations 1. Poor venting of mold at flow path ends 1. Provide effective venting in the critical regions; reduce
at the end of the flow path or at injection speed and melt temperature.
points of confluence of melt or
streams (entrapped air).
2. Confluence of several melt fronts. 2. Identify critical points at the planning stage using a
moldflow simulation for example and correct the shape,
gate location and wall thickness-distribution of the part
In both cases the air to be displaced from the mold cavity by modifications.
is highly compressed and so overheated that the plastic
melt chars locally. 3. Decrease clamp force to provide a temporary
solution.
18
9. Diesel effect
Fig. 9.1: Scorch marks due to poor mold venting at the end
of the flow path
1. The surface exhibits ejector 1. Demolding system: 1. Optimize the demolding system. Ensure sufficient num-
marks (differences in gloss, too few or incorrectly positioned ejector pins or the ber of ejector pins. Ejector pins should be placed in
stress whitening and effective surface area of the pins is too small. areas, were high demolding forces are expected (e. g.
deformation). ribs).
2. Part is damaged (punctured), 2. Undercuts, scratches or grooves. 2. Check the mold for regular surface condition and if
fractured or squashed. necessary remedy any defects.
3. Unsuitable geometry of the moldings, e.g. a highly or 3. Design the molding in line with the nature of the plastic.
disadvantageously ribbed part.
4. Shrinkage on the core during molding/cooling. Ejected 4. Cool the core more intensively. Increase cooling time,
part temperature too high. Ejector speed/pressure too reduce ejector speed/pressure.
high.
5. Overpacking the mold. 5. Increase the setting time, check the changeover from
injection pressure to holding pressure (avoid overpack-
ing) and reduce holding pressure. Enlarge the drafts.
6. Inadequate drafts. Draft not matched to the surface 6. Reduce cavity pressure through injection speed and
structure. melt temperature.
20
10. Deformation on demolding
Ejector marks
Fig. 10.1: Ejector marks due to the effective surface area of the ejector pins
being too small
Fig. 10.2: Deformed part as a result of overpacking and shrinkage onto the core
of the mold
21
11. Push marks (tiger stripes/tiger lines)
Appearance Cause Correction
Concentric, evenly spaced rings Thermoplastic multiphase systems can tend towards
radiating from the sprue which pulsating melt flow.
as a result of differences in
surface roughness appear alter- 1. Cross section of sprue and gate too small. 1. Enlarging the sprue and/or runner cross section.
nately light and dark.
2. High pressure losses in machine and hot runner nozzle. 2. Reduce pressure losses in the machine and hot runner
nozzle.
3. Wall thicknesses too low. 3. In the case of thin-walled molding with large surfaces
increasing the wall thickness often yields success.
4. Inadequate flowability of the molding compound . 4. Employ a better flowing material grade.
5. Only occasionally are unsuitable processing conditions 5. Optimize the processing parameters (high melt temper-
the cause. ature, high mold surface temperature, medium to low
injection speed and high holding pressure).
22
11. Push marks (tiger stripes/tiger lines)
a)
Fig. 11.1:
a) Tiger stripes as a result of the
sprue cross section being too
small
b) b) Remedied by enlarging the
sprue cross section
23
12. Record effect
Appearance Cause Correction
Grooved surface which propa- Melt and mold surface temperatures and injection speed Increase the melt temperature, mold surface temperature
gates along the course of the too low and flow cross section too small. and screw advance speed.
melt front. The appearance of
Enlarge the flow cross sections and optimize the shape of
this surface defect is similar to
the molding.
the grooves in a record.
Predominantly at the end of the Explanation: Reduction of the flow path lengths by means of additional
flow path. Rapid cooling of the flow front regions close to the wall sprue gates.
(frozen peripheral layer) causes the flow resistance in the
molding cavity to rise and the otherwise uniform, laminar
spread of the plastic melt to the wall to stagnate intermit-
tently. The plastic melt does not make full contact with
the mold wall.
24
12. Record effect
Molding is incompletely filled by 1. Melt temperature, mold surface temperature and injec- 1. Increase the melt and mold surface temperatures
injection. tion speed are too low. together with the injection speed.
2. Shot volume is too low, not enough material plasti- 2. Increase the shot volume and check the nonreturn valve.
cised, no melt cushion. (Shot volume too low; no melt cushion). Increase the
back pressure.
3. The injection pressure is insufficient. Machine is too 3. Match the size of the machine to the molding to be
small. produced.
4. Inadequate mold venting. 4. Improve mold venting.
5. Inadequate flowability of the plastic melt. 5. Switch to an easy flowing material grade.
6. The mold was designed with wall thicknesses which 6. Design or modify the mold to suit the material.
are too small or with long, thin-walled ribs. Flow path
too long.
7. Unfavorable nozzle bore and sprue geometry. 7. Enlarge the nozzle bore, runner and sprue cross section.
26
13. Short shot
27
14. Flash formation
Appearance Cause Correction
Moldings exhibit flash forma- 1. Fitting tolerances of the two halves of the molding are 1. Adjust mold to permissible fitting tolerances and repair
tion, e. g. at the mold parting too great or the mold parting line is damaged. existing damage in the mold parting line.
surface.
2. Clamp force of the machine is inadequate (high lifting 2. Set the clamp force higher or change to a larger
forces) or is set too low. machine.
3. Melt temperature, injection speed or internal mold 3. Lower the injection speed and holding pressure or
pressure is too high. switch earlier from injection to holding pressure.
4. Reduce melt temperature and mold temperature.
28
14. Flash formation
Fig. 14.1: Flash formation as a result of the clamp force of the machine being set too low
29
15. Jetting
Appearance Cause Correction
Generally a snake-like jet of The jet of melt shoots directly in the open cavity without
melt visible on the surface of any wall contact (no laminar flow). Since the outer skin
the molding. cools there is no longer any homogeneous connection to
the rest of the melt; the results are weld lines, inhomo-
geneities, cold forming and local internal stresses.
The strand of melt is often
rough, mat and exhibits differ-
ences in gloss or color with 1. Due to the wrong choice of gate location and design. 1. Position the gate in such a way that the jet of melt
respect to the remainder of the strikes a mold wall or a baffle plate (laminar flow).
molding. Make the gate large enough. Attachment of radii in
the transition from the gate to the molding is helpful.
2. Use higher viscosity material.
3. Profiled injection velocity (slow to normal) may provide
a temporary solution.
30
15. Jetting
Sprue
Fig. 15.1: Formation of jets of material with reference to the example of a peg Fig. 15.3: Jetting on a flat transparent part
31
16. Cold slug
Appearance Cause Correction
The surface mark often has the 1. When plastic material cools in the gating system or in 1. and 2.
appearance of a comet tail. the nozzle and arrives in the mold on the next shot. Pay attention to correct and adequate temperature con-
Because the already cooled material is not melted trol of the nozzles; make the nozzle cross section large
Easily visible in the case of
again the cold slug can also close up flow channels. enough; operate with suitably timed and adequately
thin-walled or transparent
As a result of this a division of the melt may arise with dimensioned screw retraction and reduce the back
parts.
consequent surface faults comparable to weld line faults. pressure to such an extent that escape of material from
In thick-walled parts (not the machine nozzle is prevented.
always visible) the cold slug
results in an internal flaw or in 2. An unheated or incorrectly heated machine nozzle.
a reduction of mechanical prop-
erties. 3. When, for example, the tip of the tunnel gate breaks 3. Provide a cold slug well in the runner which receives
off and lands with the next shot in the mold cavity the cold slug; as far as possible gating should not be
(only arises with brittle materials such as SAN). provided by means of a tunnel gate but rather via a hot
runner (brittle materials).
32
16. Cold slug
Fig. 16.1: Cold slug with comet tail Fig. 16.2: Cold slug in vertical illumination, enlarged
33
17. Warpage
Appearance Cause Correction
Molding exhibits deformations Due to their low shrinkage of 0.3-0.7 % substantially less
and twists (deviation from marked in styrene copolymers than in partially crystalline
desired shape). materials (shrinkage 1-3 %); in the case of glass-fiber
reinforced SAN, ABS and ASA shrinkage is reduced so far
that the lengthwise / crosswise differential is approx. 0.1 %.
As a result this effect is practically nonexistent. Terblend N
is an exception. Due to its PA6 content it tends to exhibit
higher shrinkage and is a little more susceptible to
warpage.
1. Unsuitable molding design and distinct differences in 1. Avoid internal stresses and alignments by the correct
wall thickness resulting in different internal mold pres- choice of material and parts geometry (balancing wall
sures and in different shrinkage behavior. thicknesses);
optimization of the molding with the aid of computer
programs (e. g. moldflow study).
3. Due to incorrect setting of mold temperature and injec- 3. Optimization of processing conditions.
tion speed as well as unsuitable design of mold
temperature control.
34
17. Warpage
Sprue
cold runner
Fig. 17.1: Distorted frame resulting from unfavorable part geometry (thick walled edge in this case) when the sprue position is incorrect thinwall area
35
II. Overview: Control of injection molding faults by
changing the processing parameters
Blue box
Reducing the processing parameter yields a
reduction in the injection molding fault.
Green box
In order to reduce the injection molding fault
the processing parameter must be increased or
reduced from case to case.
36
Material contamination
Screw decompression
= Increase
Material moisture
Melt temperature
(injection to hold)
Solutions
Injection speed
= Decrease
Back pressure
Hold pressure
Mold design
Clamp force
Part design
Screw rpm
= Change
Hold time
Shot size
Problems
Splay marks 2 1
Silver streaks 3 1 5 4 2
Color streaking 3 4 1 2 6 5
Delamination 2 3 1
Weld Line Appearance 1 2 3 4 5
Bubbles in part 1 2
Sink Marks 1 2 3 4 7 6 5
Voids 5 4 1 2 3 8 7 6
Mat spots/glossy spots 1 2 3 4 5 8 7 6
Crazing/stress whitening 2 1 5 3 4 7 6
Diesel effect 2 1 3 4
Sticking in Cavity 2 3 4 1
Push marks 4 3 6 5 2 1
Record effect 1 4 2 3
Short Shot 3 4 2 1 7 6 5
Flash 3 4 1 2 5
Jetting 3 4 2 1
Cold Slugs 2 1 3
Warpage 3 4 6 5 2 1
1
37
Do you have technical If you have additions or Luran SAN
questions about BASFs suggestions for this brochure Terluran ABS
styrene copolymers? please contact: Luran S ASA (ASA + PC)
Tel.: +49(0)621/60-4 29 62 Terlux MABS
We will be happy to advise you E-Mail: [email protected] Terblend N ABS + PA
at our Styrenics Infopoint:
= registered trademark of BASF Aktiengesellschaft