0% found this document useful (0 votes)
315 views

Specifications of Structural Steel and Sheet Pile

This document provides product specifications for structural steel and sheet pile, including mechanical properties and chemical compositions. It lists minimum yield points, tensile strengths, elongation percentages, and impact values for various steel types from several standards organizations. It also specifies allowable ranges and maximums for carbon, silicon, phosphorus, sulfur, and other elemental contents.
Copyright
© © All Rights Reserved
We take content rights seriously. If you suspect this is your content, claim it here.
Available Formats
Download as PDF, TXT or read online on Scribd
0% found this document useful (0 votes)
315 views

Specifications of Structural Steel and Sheet Pile

This document provides product specifications for structural steel and sheet pile, including mechanical properties and chemical compositions. It lists minimum yield points, tensile strengths, elongation percentages, and impact values for various steel types from several standards organizations. It also specifies allowable ranges and maximums for carbon, silicon, phosphorus, sulfur, and other elemental contents.
Copyright
© © All Rights Reserved
We take content rights seriously. If you suspect this is your content, claim it here.
Available Formats
Download as PDF, TXT or read online on Scribd
You are on page 1/ 8

SPECIFICATIONS

PRODUCT SPECIFICATIONS
(Structural Steel and Sheet Pile)

Mechanical Properties

Yield
Yield Point Elogation Impact
Ratio
Type of N/mm2 (min.) % (min.) J (Min.)
Classifications tensile % (max.)
Product Strength
Thickness Thickness Thickness Thickness
N/mm2
16 ≤ t ≤ t≤ 5<t t
t ≤ 16 t ≥ 12 t >12
16 5 ≤ 16 >16

245 235 400-510 - 23 18 22 27A


SM400

SM490 325 315 490-610 - 22 17 21 27A


TIS 1227 SM520 365 355 520-640 - 19 15 19 27A
1996
SS400 245 235 400-510 - 21 17 21 -

SS490 285 275 490-610 - 19 15 19 -

SS540 400 390 540 min - 16 13 17 -

SS400 245 235 400-510 - 21 17 21 -


JIS G3101
SS490 285 275 490-610 - 19 15 19 -
1995
SS540 400 390 540 min - 16 13 17 -

SM400
245 235 400-510 - 23 18 22 -
A
Structural
Steel SM400
245 235 400-510 - 23 18 22 27A
B

SM490
325 315 490-610 - 22 17 21 -
JIS G3106 A
1995 SM490
325 315 490-610 - 22 17 21 27A
B

SM490
365 355 490-610 - 19 15 19 -
YA

SM490
365 355 490-610 - 19 15 19 27A
YB

SN400 A 235 235 400-510 - 17 17 21 -

JIS G3136 235-


SN400 B 235-355 400-510 80H 18 18 22 27A
1994 335G

SN490 B 235- 325-445 490-610 80H 17 17 21 27A


445G

43A 275 265 430-580 - 20 20 20 -

43B 275 265 430-580 - 20 20 20 27B

BS 4360 43C 275 265 430-580 - 20 20 20 27A


1986 50A 355 345 490-640 - 18 18 18 -

50B 355 345 490-640 - 18 18 18 27B

50C 355 345 490-640 - 18 18 18 27A

EN 10025 S275JR 275 265 410-560 - 22 22 22 27B


1993 S355JR 355 345 490-630 - 22 22 22 27B

1997 A36 250 400-550 - 20 -

A572
1997 290 415 min - 20 -
Gr.42
ASTM
A572
1997 345 450 minE - 18 -
Gr.50

1998 A992 345-450 450 min 85D 18 -

St 33 185 175 290 - 16

St 37-2 235 225 340-470 - 24 -

DIN 17100 St 44-2 275 265 470-610 - 20 -

St 50-2 295 285 470-610 - 18 -

St 52-3 355 345 490-630 - 20 -

t < 11 11 ≤ t ≤ 40

250 260 250 410 min - 22 -

250LO 260 250 410 min - 22 -

350 360 340 480 min - 20 -


AS/NZS
350LO 360 340 480 min - 20 -
3679.1
1996 11 ≤ t
t<11 t > 17
≤ 40

300 320 300 280 440 min - 22 -

300LO 320 300 280 440 min - 22 -

JIS A5528
SY295 295 490 min - 17 -
1988,
Sheet Pile
TIS 1390-
SY390 390 540 min - 15 -
1996
Remark - Carbon Equivalent (%) = C+Mn/6 + Si/24 +Ni/40 +Cr/5 +Mo/4 +V/14 (JIS Standard)
- Carbon Equivalent (%) = C+Mn/6 + (Cr +Mo+V)/5 + (Ni +Cu)/15 (AS,ASTM Standard)
- Chemical Composition on sensitivity of welding crack =C + Si/30 +Mn/20 + Cu/20 + Ni/60 +
Cr/20 + Mo/15 + V/10 + 5B
- Bend test on material grades SS400, SS490, SS540
- Additional chemical composition controls for material under grade A992 are as follows:
Ni (max) = 0.45 , Cr (max.) =0.35 , Mo(max) =0.15 and mn/S (min.) = 20
* : Nitrogen control exclude.
SM 400 is suitable for welded structure . / เกรด SM400
เป็นเกรดทีเ่ หมาะสาหร ับโตรงสร้างทีม ่ ก ื่ ม
ี ารเชอ
- SS 400 is suitable for general structure. /เกรด SS400
เป็นเกรดทีเ่ หมาะสาหร ับโครงสร้างทวไป ่ั
SPECIFICATIONS
PRODUCT SPECIFICATIONS
(Structural Steel and Sheet Pile)

Chemical Compositions (ladle analysis)

Sensitivit
Carbon y
Classifications C Si P S Equivale of N Cu
(max. (max. Mn (max. (max. nt welding Nb V (max. (min.
) ) ) ) % crack ) )
(max.) %
(max.)

060-
SM40 0.20 0.35 0.035 0.035 - - - - - -
1.40
0

SM49 1.6
0.18 0.55 0.035 0.035 - - - - - -
0 max
TIS 1227 SM52 1.6
1996 0.20 0.55 0.035 0.035 - - - - - -
0 max

SS400 - - - 0.050 0.050 - - - - - -

SS490 - - - 0.050 0.050 - - - - - -

1.6
SS540 0.30 - 0.040 0.040 - - - - - -
max

SS400 - - - 0.050 0.050 - - - - - -

JIS G3101 SS490 - - - 0.050 0.050 - - - - - -


1995
1.6
SS540 0.30 - 0.040 0.040 - - - - - -
max

2.5x
SM40
0.23 - C 0.035 0.035 - - - - - -
0A
min.

0.60
SM40
0.20 0.35 - 0.035 0.035 - - - - - -
0B
1.40
JIS G3106 SM49 1.6
1995 0.20 0.55 0.035 0.035 - - - - - -
0A max

SM49 1.6
0.18 0.55 0.035 0.035 - - - - - -
0B max

SM49 1.6
0.20 0.55 0.035 0.035 - - - - - -
0 YA max

SM49 0.20 0.55 1.6 0.035 0.035 - - - - - -


0 YB max

SN400
0.24 - - 0.050 0.050 - - - - - -
A

0.60
JIS G3136 SN400
0.20 0.35 - 0.030 0.015 0.36 0.26 - - - -
1994 B
1.40

SN490 1.6
0.18 0.55 0.030 0.015 0.44 0.29 - - - -
B max

1.6
43A 0.25 0.50 0.050 0.050 - - - - - -
max

1.5
43B 0.21 0.50 0.050 0.050 - - - - - -
max

1.5
43C 0.18 0.50 0.050 0.050 - - - - - -
max

BS 4360 0.003 0.003


1.6
1986 50A 0.23 0.50 0.050 0.050 - - - - - -
max
0.100 0.100

1.50 0.003 0.003


50B 0.2C 0.50 C
0.050 0.050 - - - - - -
max 0.100 0.100

1.50 0.003 0.003


50C 0.2C 0.50 C
0.050 0.050 - - - - - -
max 0.100 0.100

S275J 1.5
0.21 - 0.045 0.045 - - - - 0.009* -
EN 10025 R max
1993 S355J 1.6
0.24 0.55 0.045 0.045 - - - - 0.009* -
R max

199
A36 0.26 0.40 - 0.040 0.050 - - - -
7

1.35
199 A572 F 0.01-
0.21 0.40 0.040 0.050 - - - - -
7 Gr.42 0.015
max
AST
M 1.35
199 A572 F 0.01-
0.23 0.40 0.040 0.050 - - - - -
7 Gr.50 0.015
max

0.50
199 0.10- 0.05 0.11 0.6ma
A992 0.23 - 0.035 0.045 0.45 - 0.012
7 0.40 max max x
1.50

St 33 - - - - - - - - - - -
DIN
17100 St 37-
0.17 - - 0.050 0.050 - - - - 0.009* -
2
St 44-
0.21 - - 0.050 0.050 - - - - 0.009* -
2

St 50-
- - - 0.050 0.050 - - - - 0.009* -
2

St 52-
0.2 - - 0.040 0.040 - - - - - -
3

250 0.25 0.40 - 0.040 0.040 0.43 - - - - -

1.5
250LO 0.20 0.40 0.040 0.040 0.42 - - - - -
AS/NZS max
3679.1 1.6
1996 350 0.22 0.50 0.040 0.040 0.45 - - - - -
max

1.6
350LO 0.22 0.50 0.040 0.040 0.45 - - - - -
max

1.6
300 0.22 0.50 0.040 0.040 0.44 - - - - -
max

1.6
300LO 0.22 0.50 0.040 0.040 0.44 - - - - -
max

JIS A5528 SY295 - - - 0.040 0.040 - - - - - 0.25


1998
TIS 1390- SY390 - - - 0.040 0.040 - - - - - 0.25
1996

Remark A : Impact test on material grades SM400,SM490, SM520,SM400B,SM490YB, SN400B,SN490B,


43C and 50C with thickness > 12 mm. at 0 ํC
B : Impact test on material grades 43B, 50B, S275JR with thickness > 12mm. at 20 ํC
C : It is permissible to vary the carbon and manganese contents (ladle analysis) for grades 50B
and 50C on the basis of an increase of 0.06% manganese content for each decrease of
0.01% carbon or vice versa up to maximum manganese content of 1.60% and maximum
carbon of 0.22% for grades 50B and 50C.
D : The yield radio (max.) for all thickness of materials under grades A992 is 85%
E : For grades 50 steel of thickness 20mmand under , the tensile strength shall be a minimum of
485 N/mm2.
F : A maximum of manganese of 1.50% is permissible , with an associated reduction of the
carbon maximum of 0.03%
G : For the h section, when the t1 s 9mm or less, the upper limit of the yield point or proof stress
shall not be applied.
H : For the H section , when the t1 is 9mm or less, the upper limit of the yield radio shall be 85%

- Material under TIS compulsory standard are for domestic use only , while
materials under other standards are for exportation.

SM 400 is suitable for welded structure . / เกรด SM400


เป็นเกรดทีเ่ หมาะสาหร ับโตรงสร้างทีม
่ ก ื่ ม
ี ารเชอ
- SS 400 is suitable for general structure. /เกรด SS400
เป็นเกรดทีเ่ หมาะสาหร ับโครงสร้างทวไป
่ั

TOLERANCES
TIS1227 : 1996

TIS 1227-1996

(HOT ROLLED H - SECTIONS)

Dimension Tolerance Remark

H<380 ± 2.0

Depth (H) 380≤ H<580 ± 3.0

≥ 580 ± 4.0

B<95 ± 2.0

Width (B) 95≤ B<190 ± 2.5

≥ 190 ± 3.0

t1<16 ± 0.7

t1 16≤ t1<25 ± 1.0

Thickness 25≤ t1<40 ± 1.5


(t1, t2 ) t2<16 ± 1.0

t2 16≤ t2<25 ± 1.5

25≤t2<40 ± 1.7

+ 40
L ≤ 7 m.
0
Length (L)
40+(no. of meter of L-7) x 5
L > 7 m.
0
B≤ 150 ≤1.5
H≤ 300
B> 150 ≤1.0% of B
Squareness (T)
B≤ 125 ≤1.5
H> 300
B> 125 ≤1.2% of B

H≤ 300 ≤0.15% of L To be applied to bend such as


Bend
H> 300 ≤0.10% of L sweep and camber

H≤ 300,B≤ 200 ± 2.5


Eccentricity (S)
H> 300,B> 200 ± 3.5

H<400 2.0

Concavity of web (W) 400≤H<600 2.5

H≥ 600 3.0

H≤ 187.5 ≤3.0 mm.

Squareness of cut end B≤ 187.5 ≤3.0 mm.


(e) H> 187.5 ≤1.6% of H

B> 187.5 ≤1.6% of B

t<10 ± 5% 1. The maximum thickness


shall apply.
2. These tolerances shall
apply in the purchase of a
Mass (kg/m.) single set of structural steel of
T≥ 10 ± 4% the same size and thickness
comprising not less than 10
pieces and a mass of not less
than 1,000 kg.