0% found this document useful (0 votes)
241 views

PQR Documents (01-23)

This document is a Procedure Qualification Record (PQR) that qualifies the welding procedure of a manual flux-cored arc welding (FCAW) and shielded metal arc welding (SMAW) process on a 50mm thick SA 516 Grade 70 steel joint. Tensile and bend tests met the requirements, confirming the procedure's ability to produce welds meeting the mechanical property specifications. Macro examinations showed no defects. This PQR qualifies the welding procedure for manufacturing similar joints.
Copyright
© © All Rights Reserved
We take content rights seriously. If you suspect this is your content, claim it here.
Available Formats
Download as PDF, TXT or read online on Scribd
0% found this document useful (0 votes)
241 views

PQR Documents (01-23)

This document is a Procedure Qualification Record (PQR) that qualifies the welding procedure of a manual flux-cored arc welding (FCAW) and shielded metal arc welding (SMAW) process on a 50mm thick SA 516 Grade 70 steel joint. Tensile and bend tests met the requirements, confirming the procedure's ability to produce welds meeting the mechanical property specifications. Macro examinations showed no defects. This PQR qualifies the welding procedure for manufacturing similar joints.
Copyright
© © All Rights Reserved
We take content rights seriously. If you suspect this is your content, claim it here.
Available Formats
Download as PDF, TXT or read online on Scribd
You are on page 1/ 23

-r h

~---

,r
:--

~
THERMAX
QW - 483
PROCEDURE QUALIFICATION RECORD I

(PQR)
J

Procedure Qualification Record No.: 007 - 2005 Date: 05.04.2005


WPS No.: 304-1 Rev. 3 + 003-1 Rev.6
Welding Process(es): FCAW+SMAW
Type (Manual, Automatic, Semi-Auto): MANUAL

JOINTS: (QW-402)

~ Root Gap
Root Face -
- 3 -4 mm.
-
0 1 mm.
~ )~-L[~~
IncludedAngle - 600
) 1?~

BASE METALS (QW-403) . POST WELD HEAT TREATMENT (QW-407)


Material Spec. : SA 516 to SA 516 Temperature °C : ====
Type or Grade: Gr.70 to Gr.70 Time: : ====
P. No. -1- Gr. 2 to P.No. --1-Gr.-L Others:
Thickness of Test Coupon (mm) : 50
Dia. of Test coupon (mm): Nil
Others: None GAS: (QW-408) -
% Flow
Gas(es) I Composition rate
FILLER METALS: (QW-404) Mixture lit/min
-
Process FCAW SMAW SG-C as per 18-20
Shielding CO2 SFA- 5.32
Weld Metal Analysis A.No. 1 1 Trailing None
I
Size of Filler Metal mm 0 1.2 4 Backing None
~-iller Metal F.No. 6 4
-6FA Specification 5.20 5.1
AWS Specification E71T-1 E7018 ELECTRICAL CHARACTERISTICS:(QW-409)
Deposited Weld Metal (mm) 25 25 Current: DC
Pass Thickness(mm) 4 Max. 4 Max. Polarity: EP
Others: I) No addition of supplementary filler metal & Amps: 160-180 for FCAW Volts 26-28
Alloy Elements for FCAW. 160-170 for SMAW - Volts: 23-24
ii) Product form: Flux Cored for FCAW Tungsten Electrode Type & Size: Not Applicable I
I

Others:TY"o"l'\sf'e'l M~dl. ~&\0


POSITION :(QW-405) TECHNIQUE: (QW-410)
For FCAW : 80-90
Position of Groove: ~ Travel Speed (mm/min.): For SMAW: 55-60
Welding Progression: UQhili String or Weave Bead: Strinq & Weave
Others: Oscillation:. Nil
Single pass/ Multipass: Multipass
PREHEAT :(QW-406) Single/Multiple Electrode: Sinqle
Preheat Temp. (Min.) °C : (100) Others: Weavinq for SMAW 12mm Max. (3 times
pass Temp. (Max.) °C : 250 of Core Diameter of electrode.)
Others:

[Inter .
Nil
- ~ ~.
<>
. ".f:JS
~
"'=--
Pune Office
lloyd's Register Asi..
-.

"
..
~
,r
THERMAX

. -
QW 483 PQR No. 007-2005
TENSILE TEST (QW-150)
Width Thickness Area Ultimate Tensile UTS Type of failure and
Specimen No. (mm) (mm) (mm2) load (ka.) (kg/mm2) location
TT 1 Top 19.30 26.32 507.97 31400 61.81 Ductile In PM
TT 2 Top 19.02 27.63 525.52 32000 60.89 Ductile In PM
TT 1 Bottom 18.90 26.26 496.31 31400 63.26 Ductile In PM
TT 2 Bottom 19.28 26.28 506.67 33200 65.52 Ductile In PM

GUIDED BEND TESTS (QW160)


Tvpe and Figure No. Results
. Side Bend QW-462.2 SB1 Satisfactory
Side Bend QW-462.2 SB2 Satisfactory
-...;
,..-;;:;
Side Bend QW-462.2 SB3 Satisfactory
Side Bend QW-462.2 SB4 Satisfactory

TOUGHNESS TESTS (QW 170) None


Specimen Notch Notch Test Ava. Impact Lateral Exp. Drop Weiaht
No. location Type Temp. °C Value Joules % Shear Mils Break No Break

FILLET WELD TEST (QW 180) None


Result: Not Applicable
Macro Results: ------
Micro: None --

""'"
/""

OTHER TESTS -
Type of Test: Hardness (Hv-l 0) Weld: Top: 170.179,188 Middle 185,184,187 Bottom: 194.186.179
HAZ: Top: 160.159.157 Middle: 164.163.162 Bottom: 160.160.152
Parent Material-167. 157, 160
Deposit Analysis: None
Others: Macro Test Satisfactorv.

Welder's Name: M. H. Ansari T.No.: A2932 Stamp No.: WB 01


Test Conducted by: Weldinq Enqq Dept. Lab Test No.: 226 dtd. 31.03.2005

We certify that the statements in this record are correct and that the test welds were prepared welded & tested in
accordance with the requirement of ASME Sect.lX edition 2004.

Test Witness By.: Vikas Neerai of


c-
Date: 05.04.2005 \J,\ 'f I S "" cturer: THERMAX
S LTD.
-..'V
lloyd','-"Rcgist
e]L III
siil 0::>
-,,--er ... ;......
By : V. K. SHENDRIKAR
AUDITED BY : S. A. VANCHINATH N'
.....-./
"""""
- .,

..
QW - 483
PROCEDURE QUALIFICATION RECORD
(PQR)
,r
THERMAX

Procedure Qualification Record No.: 001 - 2005 Date: 18.02.2005


WPS No.: 201-1 Rev. 5
Welding Process(es): GTAW
Type (Manual, Automatic, Semi-Auto): MANUAL

JOINTS: (QW-402)
,

\( !6 mm

RootGap - 2-3mm.
RootFace- 0 - 1.5 mm.
IncludedAngle - 65 - 70°
~

BASE METALS (QW-403) POST WELD HEAT TREATMENT (QW-407) Nil -


Material Spec. : SA 516 to SA 516 Temperature°C: =
Type or Grade: r.70 to Gr.70 Time: ---------
....1.- Gr.
P. ,'-10. 2 to P.No.-1- Gr. 2 Others: ---------
Thickness of Test Coupon (mm) : 16
Dia. of Test coupon (mm): Nil.
Others: None
GAS: (QW-408)
% Flow
Gas(es) Composition rate
l Mixture lit/rnin
FILLER METALS: (QW-404) I ---
Process GTAW Shielding As per 10-11
GTAW Argon SFA 5.32
Weld Metal Analysis A.No. 1 Trailing None ---- ----
Size of Filler Metal mm 0 2 Backing None ---- ----
Filler Metal F.No. 6 -,-
--"'"
I SFA Specification 5.18 --.
. AWS Specification ER 70S-2 ELECTRICAL CHARACTERISTICS:(QW-409)
Deposited Weld Metal (mm) 16 Current: DC
Pass Thickness(mm) 3 Max. Polarity: EN
Others No addition of flux to Amps: 140-150 Volts N.A
The face of weld joint Tungsten Electrode Type & Size: EWTh-2. .,])2.4
Others: Nil
-
POSITION :(QW-405) TECHNIQUE: (QW-410)
Position of Groove: Travel Speed: -----
Welding Progression: ------- String or Weave Bead: StrinQ & Weave
Others: --------- Oscillation: Nil
. I Single pass/ Multipass: Multipass
PREHEAT :(QW-406) I Single/Multiple Electrode: SinQle -
PreheatTemp.(Min.)°C : RT (28) Others: Nil
InterpassTemp.(Max.)°C : 250
Others:

Nil." --.I \('4'">


...."' "... I
; \.~
,'& '- ~
I

I
~
~J . p
1

,
,r
THERMAX

QW 483 PQR No. 001-2005


TENSILE TEST (QW-150)
Width Thickness Area Ultimate Tensile UTS Type of failure
Specimen No. (mm) (mm2) load (ka.)
(mm) (kg/mm2) and location -
Trans. Tensile 1 19.40 15.97 309.82 19800 63.91 Ductile In PilJl
Trans. Tensile 2 19.33 16.09 311.02 19800 63.66 Ductile In PM

GUIDED BEND TESTS (QW 160)


Type and FiQureNo. Results
Face Bend QW-462.3 (a) FB1 Satisfattory
Face Bend QW-462.3 (a) FB2 Satisfactory
Root Bend QW-462.3 (a) RB1 Satisfactory
..-
Root Bend QW-462.3 (a) RB2 Satisfactory

TOUGHNESS TESTS (QW 170)


Specimen Notch Notch Test Ava. Impact Lateral Exp. Drop Weiaht
No. location Type Temp. °C Value Joules % Shear Mils Break No Break
-
1-3 weld -29 110

HAZ
1-3
} Charpy
-29 28

FILLET WELD TEST (QW 180) None


Result: Satisfactory Yes/No.
Macro Results: None
Micro: None --

........ OTHER TESTS


i"ype of Test: Hardness (Hv10). Weld - 194, 198,186. HAZ-199,197,185.
Parent Material - 176,181,171.
Deposit Analysis: None
Others: Macro -Satisfactory ...-

Welder's Name: M. H. Ansari T.No.: A2932 Stamp No.: WB01


Test Conducted by: WeldinQ EnQQDept. Lab Test No.: 199 dtd. 10.02.2005

We certify that the statements in this record are correct and that the test welds were prepared welded & tested in
accordance with the requirement of ASME SecUX edition 2004.

Test Witness By.: Vikas Neerai of LRS

Date: 18.02.2005 Manufacturer: THERMAX LTD.

AUDITED y' 4: 5, ('


\.
n <:)
V. K. SHENDRIKAR

~A~~ ,~. , .

\
~ \ 0 ~)/ ~~i.ter Asia
iF""
rr ....
I
t..

,r
~
~

QW - 483 THERMAX
PROCEDURE QUALIFICATION RECORD
(PQR)

ProcedureQualificationRecordNo.: 005- 2004 Date: 14.05.2004


WPS No.:- 201-1Rev.4
WeldingProcess(es): GTAW
Type(Manual,Automatic,Semi-Auto): MANUAL

JOINTS: (QW-402)

-~
+ \( E74 mm

Root Gap ---- 3.0 to 3.5 mm.


RootFace--- 0 to 1mm.
IncludedAngle- 70-75°

BASE METALS (QW-403) POST WELD HEAT TREATMENT(QW-407) Nil


Material Spec.: SA 106 to SA 106 Temperature DC: ----------
Type or Grade: Gr.B to Gr.B Time: ----------
P No 1 Gr.A- to P.No. --L- Gr. .1.. Others: ----------
Thickness of Test Coupon (mm): 8.74
Dia. of Test coupon (mm): 60.3.
Others: None
GAS: (QW-408)
% Flow
Gas(es) Composition rate
FILLER METALS: (QW-404) Mixture lit/min
Process GTAW Shielding Argon As per 8-10
GTAW SFA 5.32
r-... Weld Metal Analysis A.No. 1 Trailing None ---- ----
Size of Filler Metal mm 0 2 Backing None - -
Filler Metal F.No. 6
SFA Specification 5.18
AWS Specification ER 70S-2 ELECTRICAL CHARACTERISTICS:(QW-409)
Deposited Weld Metal (mm) 8.74 Current: DC
Pass Thickness(mm) 3 Max. Polarity: EN
Others No addition of flux to Amps: 100-120 Volts N.A
The face of weld joint Tungsten Electrode Type & Size: EWTh-2. g,2.j
Others: Nil

POSITION :(QW-405) TECHNIQUE: (QW-410)


Position of Groove: 1G Travel Speed: -----
Welding Progression: ------ String or Weave Bead: Strinq & Weave
Others: ---------- Oscillation: WL
Single pass/ Multipass Multipass
PREHEAT :(QW-406) Single/Multiple Electrode: Sinqle
Preheat Temp. DC: RT (39) Others: Nil
_/ 250
Interpass Temp. DC:
Others: Nil

0 t-4.J- -
JEj'cY
, .... t~
".

,r
..
. ,

THERMAX

QW 483 PQR No. 005-2004


TENSILE TEST (QW-150)
Specimen Area Ultimate Tensile
No. mm2 load k .
TT-1 159.00 7850

TT-2 19.35 8.79 170.09 8250 48.52

."""
Results
Satisfacto
Satisfacto
Satisfacto
Satisfacto

Specimen Notch Notch Dro


No. location Type Break

FILLET WELD TEST (QW 180) None


~
Result: Satisfactory Yes/No.
Macro Results: None
Micro: None
OTHER TESTS
Type of Test: Hardness (Hv). Weld 180. 189. 199. HAZ- 193. 191. 186.
Parent Material-197. 194. 193.
Deposit Analysis: None
Others:

Welder's Name: M.H.Ansari T.No.: A2932 Stamp No.: WB 01


Test Conducted by: Weldin!:! Ena!:! DeDI. Lab Test No.: 27 dtd. 14.05.2004

We certify that the statements in this record are correct and that the test welds were prepared welded &
tested in accordance with the requirement of ASME SecUX edition 2001 including addenda 03.

Test Witness By.: Surveyor of LRA

Date: 14.05.20°L\- cturer: THERMAX LTD.

~.
~",,4
AUDITED BY : SA VANCHINATH
By : A.H.Jadhav

L
-r h
~---

,r
:--

~
THERMAX
QW - 483
PROCEDURE QUALIFICATION RECORD I

(PQR)
J

Procedure Qualification Record No.: 007 - 2005 Date: 05.04.2005


WPS No.: 304-1 Rev. 3 + 003-1 Rev.6
Welding Process(es): FCAW+SMAW
Type (Manual, Automatic, Semi-Auto): MANUAL

JOINTS: (QW-402)

~ Root Gap
Root Face -
- 3 -4 mm.
-
0 1 mm.
~ )~-L[~~
IncludedAngle - 600
) 1?~

BASE METALS (QW-403) . POST WELD HEAT TREATMENT (QW-407)


Material Spec. : SA 516 to SA 516 Temperature °C : ====
Type or Grade: Gr.70 to Gr.70 Time: : ====
P. No. -1- Gr. 2 to P.No. --1-Gr.-L Others:
Thickness of Test Coupon (mm) : 50
Dia. of Test coupon (mm): Nil
Others: None GAS: (QW-408) -
% Flow
Gas(es) I Composition rate
FILLER METALS: (QW-404) Mixture lit/min
-
Process FCAW SMAW SG-C as per 18-20
Shielding CO2 SFA- 5.32
Weld Metal Analysis A.No. 1 1 Trailing None
I
Size of Filler Metal mm 0 1.2 4 Backing None
~-iller Metal F.No. 6 4
-6FA Specification 5.20 5.1
AWS Specification E71T-1 E7018 ELECTRICAL CHARACTERISTICS:(QW-409)
Deposited Weld Metal (mm) 25 25 Current: DC
Pass Thickness(mm) 4 Max. 4 Max. Polarity: EP
Others: I) No addition of supplementary filler metal & Amps: 160-180 for FCAW Volts 26-28
Alloy Elements for FCAW. 160-170 for SMAW - Volts: 23-24
ii) Product form: Flux Cored for FCAW Tungsten Electrode Type & Size: Not Applicable I
I

Others:TY"o"l'\sf'e'l M~dl. ~&\0


POSITION :(QW-405) TECHNIQUE: (QW-410)
For FCAW : 80-90
Position of Groove: ~ Travel Speed (mm/min.): For SMAW: 55-60
Welding Progression: UQhili String or Weave Bead: Strinq & Weave
Others: Oscillation:. Nil
Single pass/ Multipass: Multipass
PREHEAT :(QW-406) Single/Multiple Electrode: Sinqle
Preheat Temp. (Min.) °C : (100) Others: Weavinq for SMAW 12mm Max. (3 times
pass Temp. (Max.) °C : 250 of Core Diameter of electrode.)
Others:

[Inter .
Nil
- ~ ~.
<>
. ".f:JS
~
"'=--
Pune Office
lloyd's Register Asi..
-.

"
..
~
,r
THERMAX

. -
QW 483 PQR No. 007-2005
TENSILE TEST (QW-150)
Width Thickness Area Ultimate Tensile UTS Type of failure and
Specimen No. (mm) (mm) (mm2) load (ka.) (kg/mm2) location
TT 1 Top 19.30 26.32 507.97 31400 61.81 Ductile In PM
TT 2 Top 19.02 27.63 525.52 32000 60.89 Ductile In PM
TT 1 Bottom 18.90 26.26 496.31 31400 63.26 Ductile In PM
TT 2 Bottom 19.28 26.28 506.67 33200 65.52 Ductile In PM

GUIDED BEND TESTS (QW160)


Tvpe and Figure No. Results
. Side Bend QW-462.2 SB1 Satisfactory
Side Bend QW-462.2 SB2 Satisfactory
-...;
,..-;;:;
Side Bend QW-462.2 SB3 Satisfactory
Side Bend QW-462.2 SB4 Satisfactory

TOUGHNESS TESTS (QW 170) None


Specimen Notch Notch Test Ava. Impact Lateral Exp. Drop Weiaht
No. location Type Temp. °C Value Joules % Shear Mils Break No Break

FILLET WELD TEST (QW 180) None


Result: Not Applicable
Macro Results: ------
Micro: None --

""'"
/""

OTHER TESTS -
Type of Test: Hardness (Hv-l 0) Weld: Top: 170.179,188 Middle 185,184,187 Bottom: 194.186.179
HAZ: Top: 160.159.157 Middle: 164.163.162 Bottom: 160.160.152
Parent Material-167. 157, 160
Deposit Analysis: None
Others: Macro Test Satisfactorv.

Welder's Name: M. H. Ansari T.No.: A2932 Stamp No.: WB 01


Test Conducted by: Weldinq Enqq Dept. Lab Test No.: 226 dtd. 31.03.2005

We certify that the statements in this record are correct and that the test welds were prepared welded & tested in
accordance with the requirement of ASME Sect.lX edition 2004.

Test Witness By.: Vikas Neerai of


c-
Date: 05.04.2005 \J,\ 'f I S "" cturer: THERMAX
S LTD.
-..'V
lloyd','-"Rcgist
e]L III
siil 0::>
-,,--er ... ;......
By : V. K. SHENDRIKAR
AUDITED BY : S. A. VANCHINATH N'
.....-./
\ QW - 482
WELDING PROCEDURE SPECIFICATION
(WPS)
,r
THERMAX

Welding Procedure Specification No. : 201-2 Rev. Q Date 20.03.2008

Welding Process (es): GTAW Type(s): Manual PQR No. : 001/2005, 005/2004

JOINTS: (QW-402) Details

Joint Design: As per equipment Drawinq & Refer to relevant WTS.

Backing: No for root pass, Yes for subsequent passes.

Backing Material (Type): Base metal of P1 / Weld metal.

::J Metal 0 Nonfusing Metal


.-.. Nonmetallic 0 Others
Retainers not permitted
BASE METALS: (QW-403) FILLER METAL: (QW-404)
Process GTAW
P.NO. 1 Gr. 1 , 2 to P.No. 1 Gr 1 , 2 .
OR F.No. 6
-------
Specification Type & Grade
To A.No. 1

Specification Type & Grade


OR SFA No. 5.18

Chem. Analysis & Mech. Prop. n-

To AWS(Class) ER 70S-2
---
Chem. Analysis & Mech. Prop.
Product form (Solid/cored / Solid
Flux cored) GTAW / PAW
-- Size of Filler metal (mm) 0 2.0,

GROOVE FillET Electrode-Flux (Class) Not


Base Metal 1.5 - 32 Any Applicable
thk.range (mm.) Trade Name (Flux) Not

Pipe dia Any Any Applicable


Range (mm.) Consumable Insert None

Others: This WPS is applicable for base metal Deposited weld Groove 32

Without Notch Toughness requirements. metal Thk. range Fillet Any


(mm.)
Pass Thk. (mm.) :::;3
Others: No addition of flux to the face of weld joint.

,'~
~

You might also like