0% found this document useful (0 votes)
173 views

CSWIP Visual Inspection PIPE REPORT

This 3 page document is a visual inspection report for a pipe welding job. It contains details of the welding process used, measurements and observations of defects found on the external and internal weld faces and root sections. Photographs show issues like undercut, lack of root penetration, poor toe blend and stray flash. The inspector found defects like undercut up to 1.5mm deep, poor root formation, grinding marks and spatter on the pipe.

Uploaded by

Naga Rajan
Copyright
© © All Rights Reserved
We take content rights seriously. If you suspect this is your content, claim it here.
Available Formats
Download as PDF, TXT or read online on Scribd
0% found this document useful (0 votes)
173 views

CSWIP Visual Inspection PIPE REPORT

This 3 page document is a visual inspection report for a pipe welding job. It contains details of the welding process used, measurements and observations of defects found on the external and internal weld faces and root sections. Photographs show issues like undercut, lack of root penetration, poor toe blend and stray flash. The inspector found defects like undercut up to 1.5mm deep, poor root formation, grinding marks and spatter on the pipe.

Uploaded by

Naga Rajan
Copyright
© © All Rights Reserved
We take content rights seriously. If you suspect this is your content, claim it here.
Available Formats
Download as PDF, TXT or read online on Scribd
You are on page 1/ 4

Page 1 of 3 CSWIP VISUAL INSPECTION PIPE REPORT

Name [Block capitals] _______________________ Signature_______________ Pipe Ident#__________

Code/Specification used_____________________ Welding Process__________ Joint type____________

Welding position________________________ Outside ∅ & Thickness_______ Date ________________

WELD FACE

A B C

C D A

P.T.O. [ FOR ROOT]


Page 2 of 3

PIPE ROOT FACE

A B C

C D A
Visual Inspection Pipe Report
Name [Block capitals]_ ___Signature _____Pipe Ident__E9___

Code/Specification used YOUR CODE Welding Process____MMA__Joint type Single V

Welding position_____5G___________Outside Ø and Thickness_mm Date_

Weld face

Cap height 6 max Cap height 5 max


Cap width 17-20 Cap width 16-20
Toe blend poor Toe blend poor
Stray Hi/lo 1mm
flash
A B C
70 3
27

5 1
10 48 138
3
25 Poor Undercut
0.5 sharp

Stray flash

Light spatter both


B sides C

Smooth mechanical markings and pitting < 0.5mm deep is evident throughout parent materials over whole pipe

Cap height 4 max Cap height 3.5 max


Cap width 17-20 Cap width 19-24
Toe blend poor Toe blend smooth

Grinding
Poor 0.5 smooth
restart +
C overlap D A
15
72
132 48

Hammer 12
mark 118 10
1 deep 104 34
Arc
smooth strike
15 65 6
14 Grinding
3 20 0.5 smooth
16 Grinding
0.5 deep
Arc strike smooth

pto [for root]


Pipe Ident__E9___

Pipe root face

Spatter Penetration height 4


Penetration width 6-8
8 Toe blend poor
2 Hi/lo 1 mm
8

A Root undercut B Very poor root C


0.5 deep sharp formation

56 4 55 31

62 1 10 5 5
20 81 90 54 86
Poor pickup
Root undercut Root undercut Root undercut Root undercut
1 deep sharp 0.5 deep 0.5 deep 0.5 deep
sharp sharp sharp
Penetration height 3.5
Penetration width 7-8
Toe blend poor
Hi/lo 1.5mm

108 4

Root undercut Root undercut 93 2 Spatter


0.5 deep 0.5 deep
sharp sharp
C D A
Spatter
23 2 109 3

9 5 28
19 72 69

Root undercut Root undercut Root undercut


<1 deep sharp <1 deep sharp 0.5 deep smooth

Penetration height 4 Penetration height 2


Penetration width 6-8 Penetration width 6-8
WELD INSPECTION REPORT/SENTENCE SHEET
Toe blend poor Toe blend smooth