This document provides specifications for a material called BS970-3:1991 (Gr.817M40). It includes: 1. Chemical composition requirements for elements like carbon, silicon, manganese, and chromium. 2. Mechanical properties for the material in different conditions ('T', 'U', 'V') including minimum yield strengths, tensile strengths, and hardness values. 3. Heat treatment temperature requirements and processes for normalizing, quenching, and tempering the material to achieve the specified conditions and properties.

Uploaded by

Lionell Logesh
Copyright
© © All Rights Reserved
We take content rights seriously. If you suspect this is your content, claim it here.
Available Formats
Download as PDF, TXT or read online on Scribd
0% found this document useful (0 votes)
132 views

TDC En24

This document provides specifications for a material called BS970-3:1991 (Gr.817M40). It includes: 1. Chemical composition requirements for elements like carbon, silicon, manganese, and chromium. 2. Mechanical properties for the material in different conditions ('T', 'U', 'V') including minimum yield strengths, tensile strengths, and hardness values. 3. Heat treatment temperature requirements and processes for normalizing, quenching, and tempering the material to achieve the specified conditions and properties.

Uploaded by

Lionell Logesh
Copyright
© © All Rights Reserved
We take content rights seriously. If you suspect this is your content, claim it here.
Available Formats
Download as PDF, TXT or read online on Scribd
You are on page 1/ 2

NCON TURBO TECH PVT LTD

# F-62 & F-63, Industrial Estate, Rajaji nagar


Bangalore – 560044

EN 24
1. TDC No : TDC/General/01 Prelim.00. Dt.23.04.2022
2. Material Specification : BS970-3 : 1991 (Gr.817M40)

CHEMICAL PROPERTIES

Composition%
Element
Minimum Maximum
Carbon 0.36 0.44
Silicon 0.10 0.40
Manganese 0.45 0.70
Phosphorous --- 0.035
Sulfur --- 0.04
Chromium 1.00 1.40
Molybdenum 0.20 0.35
Nickel 1.30 1.70

MECHANICAL PROPERTIES

Description ‘T’ Condition ‘U’ Condition ‘V’ Condition


Yield Strength (MPa) 650 min 755 min 850
0.2 %Proof Strength (MPa) 665 min 740 min 835
Tensile Strength (Mpa) 850-1000 925-1075 1000 – 1150
Elongation (%) 13 12 12
Hardness (BHN) 248 – 302 269-331 292-352
1. Charpy : 35 1. Charpy : 42 1. Charpy : 42
Impact at RT (J)
2. Izod : 40 2. Izod : 47 2. Izod : 47

Page 1 of 2
NCON TURBO TECH PVT LTD
# F-62 & F-63, Industrial Estate, Rajaji nagar
Bangalore – 560044

EN 24
1. TDC No : TDC/General/01 Prelim.00. Dt.23.04.2022
2. Material Specification : BS970-3 : 1991 (Gr.817M40)

HEAT TREATMENT TEMPERATURE

Cooling
Process ‘T’ Condition ‘U’ Condition ‘V’ Condition Holding Time
Medium
Holding time
Normalizing 840 840 840 Air 1 min. /mm of
thickness.
Holding time
Quenching 850 – 860 850-860 850-860 Oil 1 min. /mm of
thickness.
Holding time
2.5 min. /mm
Tempering 660 630 610 Air
of thickness.
Or min. 1 hrs.

Notes:

1. The Heat Treatment Process flow should be Normalizing, Rough Machining, Quenching, and Tempering followed by
Proof Machining.
2. UT should be carried out as per ASTM A388 straight beam examination using DGS scale with acceptance of Ø3 mm
FBH or equivalent.
3. The Hardness variation of the Final Component should be maximum of 20 BHN.