The document provides the results of a tensile test on a steel sample with a thickness of 6mm. The test was conducted according to EN ISO 4136. Specimens 1 and 2 both had a yield point around 328-332 MPa and tensile strength around 451-453 MPa.
Copyright
© © All Rights Reserved
We take content rights seriously. If you suspect this is your content, claim it here.
Available Formats
Download as PDF, TXT or read online on Scribd
0% found this document useful (0 votes)
32 views

Tensile Test

The document provides the results of a tensile test on a steel sample with a thickness of 6mm. The test was conducted according to EN ISO 4136. Specimens 1 and 2 both had a yield point around 328-332 MPa and tensile strength around 451-453 MPa.
Copyright
© © All Rights Reserved
We take content rights seriously. If you suspect this is your content, claim it here.
Available Formats
Download as PDF, TXT or read online on Scribd
You are on page 1/ 1

TENSILE TEST CERTIFICATE

G8/DTR51(20/1/2001)

Test No: 3294 Page: 1 from 1


Report No: T23.740.TT001 Date: 02/5/2023
Testing machine: AVERY 7104DCJ Filler metal 1: -
Sample received date: 24/04/2023 Filler metal 2: -
Client: AXIONTEK Diameter: -
Client address: Thickness: 6mm
Contractor: - Procedure: -
Project: PQR Test according to: EN ISO 4136
Material: - Test temperature: -
Material type: S275 JR Comments: -

Specim.N Specimen dimensions/ diameter Yield Point Tensile strength Elong 70 Failure Remarks
o Lo= Character
(W) mm ( t)mm Area mm2 KN MPa KN MPa mm % Location

1 25,0 6,0 150,0 49,2 328 67,7 451 87,0 24,3 BASE METAL
2 25,0 6,0 150,0 49,7 332 68,0 453 87,0 24,3 BASE METAL
3 - - - - - - - - -
4 - - - - - - - - -

80 80
68,0
67,7

70 70

60 60
49,7
49,2

50 50

40 40

30 30

20 20

10 10

0 0
0 100 200 300 400

Witnessed: Note: The Test is for: For GATS:


-- A. STRANTZAS
Welding Procedure qualification
Welder's Qualification