Helios Firing Schedules - FAHRENHEIT - Page 4
Helios Firing Schedules - FAHRENHEIT - Page 4
The following schedules were built for Bullseye glass based on decades of
experience and testing published by Bullseye, knowledge published by artists who
use BE glass, and personal experience collected from the kilns at Helios. We
adjust these schedules based on which kiln we are using and the needs of each
project. Make adjustments for your own specific kiln and for each specific project. All temperatures
are in degrees FAHRENHEIT.
FULL - 1 Layer - 3mm thick FULL - 2 Layers - 6mm thick TIPS to adjust your
schedule
Ramp Temp Hold Ramp
(*F per (*F per
Temp Hold
hr)
(*F) (hrs:min)
hr)
(*F) (hrs:min) Increase or decrease the
processing temperature
1 300 1000 :15 1 300 1000 :15 (segment 3) based on how
2 100 1225 :30 2 100 1225 :30 your kiln fires and how much
the glass needs to move.
3 Full 1490 :10 3 Full 1490 :10
4 Full 900 :45 4 Full 900 :60 For non-BE glass, change the
annealing temperature
5 200 800 :00 5 100 800 :00 (segment 4) and following
6 300 700 :00 6 200 700 :00 segments according to the
manufacturer of the glass.
7 0 7 300 200 :00
8 0 For textured pieces, or
thicker than 12mm, change
initial ramp, anneal hold, and
cooling segments (segments
FULL - 3 Layers - 9mm thick FULL - 4 Layers - 12mm thick 4-7) using Bullseye Thick
Slabs Annealing chart.
Ramp Temp Hold Ramp
(*F per (*F per
Temp Hold Add segments if your project
(*F) (hrs:min) (*F) (hrs:min)
hr) hr)
needs:
1 250 1000 :15 1 200 1000 :15 ◆ Expel moisture
2 100 1225 :30 2 100 1225 :30 ◆ Expel binders/glue
3 Full 1490 :10 ◆ Pink Hold
3 Full 1490 :10
◆ Double Bubble Squeeze
4 Full 900 1:30 4 Full 900 2:00 ◆ Pre-Anneal Hold
5 75 800 :00 5 50 800 :00
For larger than 10in x 10in,
6 150 700 :00 6 100 700 :00 use the next thicker schedule.
7 250 200 :00 7 200 200 :00 Go another layer up for every
8 0 8 0 4in larger.