The following schedules were built for Bullseye glass based on decades of
experience and testing published by Bullseye, knowledge published by artists who
use BE glass, and personal experience collected from the kilns at Helios. We
adjust these schedules based on which kiln we are using and the needs of each
project. Make adjustments for your own specific kiln and for each specific project. All temperatures
are in degrees FAHRENHEIT.
TACK - 1 Layer - 3mm thick TACK - 2 Layers - 6mm thick TIPS to adjust your
schedule
Ramp Temp Hold Ramp Temp Hold
(*F per (*F per
hr)
(*F) (hrs:min)
hr)
(*F) (hrs:min)
Increase or decrease the
processing temperature
1 300 1000 :15 1 300 1000 :15 (segment 3) based on how
2 100 1225 :30 2 100 1225 :30 your kiln fires and how much
the glass needs to move.
3 Full 1325 :10 3 Full 1325 :10
4 Full 900 :45 4 Full 900 :60 For non-BE glass, change the
annealing temperature
5 200 800 :00 5 100 800 :00
(segment 4) and following
6 300 700 :00 6 200 700 :00 segments according to the
7 0 7 300 200 :00 manufacturer of the glass.